About Us About Us
News

Industry standards and process requirements for bimetallic hammer heads

2025-07-17 103

The industry standards and process requirements for bimetallic hammer heads involve multiple aspects such as material selection, heat treatment processes, and quality control. The following is a comprehensive summary of key information:

image.png

1、 Industry standards and specifications

Material standards

The high chromium alloy working area must comply with the KmTBCr28 or higher grade, with a hardness requirement of HRC ≥ 55-60 and a thickness deviation of the wear-resistant layer ≤+1.5mm.

If seamless steel pipes are used for the outer pipe (hammer handle), they must meet the mechanical performance requirements of GB/T 8163-2008 (Seamless Steel Pipes for Fluid Transport).

Process standards

The composite casting process shall comply with GB/T 5680-2010 (High Chromium Cast Iron Parts) or the power industry standard DL/T 680-2015 (Acceptance Specification for Wear resistant Parts).

The heat treatment process needs to be verified for welding and composite layer quality through JB/T 4730-2005 (Non destructive Testing of Pressure Equipment).

2、 Core process requirements

Heat treatment process

High chromium alloy section:

The quenching temperature is 950-1150 ℃ (air-cooled or oil cooled), forming a martensitic matrix (HRC 58-65), and the wear resistance is improved by 3-5 times.

Tempering temperature of 200-300 ℃, eliminating internal stress and improving toughness by more than 30%.

Hammer handle part:

Low alloy steel requires normalizing (850-900 ℃) and tempering (550 ℃) to maintain toughness (HRC 37-44).

Composite process control

Adopting dual liquid composite casting or lost foam vacuum casting to ensure the bonding strength between high chromium alloy and hammer handle.

After casting, softening annealing (650-750 ℃) is required to eliminate shrinkage/cracks before machining.

Special process optimization

Salt bath local treatment: The installation end of the hammer head is treated in a salt bath at 640-660 ℃ to improve toughness by 30%.

High frequency quenching: suitable for thin-walled hammer heads, fast heating reduces oxidation, and the surface hardness is uniform.

3、 Key points of quality control

Defect prevention and control

Insufficient quenching can result in soft spots on the surface and a 60% reduction in lifespan; Insufficient tempering can easily cause brittle cracking in the core.

Cooling medium selection: High chromium alloys are preferred for air cooling, while low-alloy steels require controlled water temperature (≤ 30 ℃) to prevent cracking.

Testing requirements

Wear resistant layer hardness testing (HRC ≥ 55), metallographic analysis (uniformity of carbide distribution), and impact testing (≥ 12 J/cm ²).

Non destructive testing (such as ultrasonic testing) shall comply with JB/T 4730-2005.

4、 Applicable scenarios and selection suggestions

High impact working conditions (such as crushed granite): It is recommended to use high chromium alloy quenching and salt bath strengthening to increase the service life by 5-8 times.

Medium impact condition: Segmented quenching of low-alloy steel (HRC 54-61) can extend its service life by 2-3 times.

For further understanding of specific process parameters or equipment selection, please refer to relevant industry standard documents or manufacturer technical manuals.