About Us About Us
News

What issues should be noted in the tempering treatment of Tiankuo bimetallic hammer heads?

2025-03-24 91

The tempering treatment of Tiankuo bimetallic hammer head is a key step to ensure its wear resistance and toughness balance, and special attention should be paid to the following core issues, integrating process points from multiple sources:

image.png

1、 Accurate temperature control

Low temperature tempering range

The tempering temperature usually needs to be strictly controlled at 200-300 ℃ (such as 250 ℃± 20 ℃ or 300 ℃± 20 ℃). If the temperature is too high, it will reduce the hardness of the working part of the hammer head, and if it is too low, it will not be able to fully eliminate quenching stress.

Note: The specific temperature needs to be adjusted according to the material composition. For example, the composite interface between high chromium cast iron (Cr 15-35%) and carbon steel should avoid cracking caused by thermal expansion differences.

Segmented heating for crack prevention

For large hammer heads, it is recommended to use segmented heating (such as heating to 670 ℃ for insulation first, and then raising to the target tempering temperature) to avoid stress cracks caused by temperature gradients.

2、 Time and cooling method

Adequate insulation time

The insulation time should be 3-5 hours (adjusted according to the size of the hammer head) to ensure sufficient release of internal stress. Too short may result in residual stress, while too long may reduce efficiency.

Example: Tiankuo casting process requires 250 ℃ tempering and insulation for 3-5 hours.

Mainly air cooling

After tempering, air cooling must be used (water cooling or oil cooling is prohibited) to avoid new thermal stress or cracks caused by rapid cooling.

Special reminder: The lost foam casting hammer head needs to be naturally cooled to room temperature in air.

3、 Interface and Operational Risk Prevention and Control

Interface combination protection

The tempering process needs to ensure that the bimetallic interface is firmly bonded to avoid delamination caused by differences in shrinkage rates between the two metals. Preheating and gradual cooling are effective means to reduce interface stress.

Operating Specifications

The surface of the hammer head needs to be cleaned and polished to avoid residual oxide skin or crack defects;

The temperature uniformity of the heat treatment furnace needs to be calibrated regularly to prevent local overheating.

summary

The core of tempering Tiankuo bimetallic hammer head is "precise temperature control+sufficient insulation+slow cooling", which requires dynamic adjustment of parameters according to material composition (such as Cr content), casting process (sand mold/lost foam) and hammer head size. In practical operation, it is recommended to conduct small-scale trial processing based on equipment conditions, optimize the process, and then proceed with large-scale production.

>Safety reminder: After tempering, the hammer head should be placed in a dry environment to avoid hydrogen embrittlement (especially for high chromium cast iron)