About Us About Us
News

Quality standard specification for bimetallic hammer heads

2024-09-12 107

Specification for Quality Standards of Bimetallic Hammer Heads (Current Effective Technical System)

1. Current mandatory national standards

GB/T 26652-XXXX "Wear resistant Composite Material Castings" (2024 revised draft, has been released for comments, will soon replace GB/T 26652-2011)

Scope of application: Suitable for wear-resistant composite material castings in industries such as mining, metallurgy, building materials, power, and chemical, covering products such as bimetallic hammers, liners, roller sleeves, etc.

Core update content:

Clearly define "liquid-liquid composite one-time casting" as the only legal composite process, and prohibit non metallurgical bonding methods such as welding, embedding, and bonding;

Add metallographic judgment requirements for "gradient distribution of transition zone elements", requiring Cr, Mn, C and other elements to exhibit continuous gradient changes at the interface without obvious interface cracks or slag inclusions;

Refine the "hardness distribution" detection method, requiring multi-point Rockwell hardness (HRC) measurements to be taken separately for the working end and hammer handle, and drawing a hardness gradient curve;

Introduce the minimum limit of "impact toughness": hammer handle area ≥ 12J/cm ² (tested according to GB/T 229 standard);

It is stipulated that a spectral analysis report (Cr ≥ 15%, Mn ≥ 1.0%, S ≤ 0.03%), an ultrasonic flaw detection report (without internal shrinkage or cracks), and a metallographic structure chart (grain size ≤ 5) must be provided before leaving the factory.

Standard status: The current valid version is GB/T 26652-XXXX, and the original GB/T 26652-2011 has been abolished.

2. Core industry reference standards

|Standard Number | Standard Name | Key Technical Requirements | Application Scenarios|

|GB/T 24187-2009 | "High Chromium Cast Iron" | - Working end Cr content: ≥ 15% (recommended Cr18-26%) - Hardness: HRC ≥ 58 (measured ≥ 60 is preferred) - Impact toughness: ≥ 12J/cm ² - Metallographic structure: Martensite+carbides, no network carbides | Basis for determining the working end material of bimetallic hammer heads|

|DL/T 680-2015 | Technical Conditions for Wear resistant Pipelines in the Power Industry | - Composite Layer Cr ≥ 28%, Ni ≥ 1.0% - Hardness HRC ≥ 58- Wear resistant Layer Thickness ≥ 5mm | Reference for Hammer Selection of Coal Mill in Power Systems|

|GB/T 229 | "Charpy Pendulum Impact Test Method for Metallic Materials" | Used for testing the impact toughness of hammer handle, sample size: 10 × 10 × 55mm, temperature: 20 ± 5 ℃ | As a supporting testing standard for GB/T 26652-XXXX|

✅  Note: Although GB/T 24187-2009 is not a specialized standard for hammer heads, it is widely used as the core material judgment basis in the industry due to its systematic regulations on the composition and performance of high chromium cast iron.

3. Quality inspection methods and verification processes

Hardness testing

Tool: Rockwell hardness tester (HRC)

Method:

Work end: Measure at least 5 points on the polished surface, take the average, and require HRC 58-65;

Hammer handle: Measure the neck of the hammer, requiring HRC 30-40 to avoid brittle fracture due to excessive hardness.

Prohibited behavior: Only detect a surface depth of 1mm and use Brinell hardness (HB) instead of HRC.

Metallographic structure analysis

Requirement: Cut the cross-section, polish and corrode it, and observe it under an optical microscope

Working end: Martensite+carbide (Cr ₇ C ∝, Cr ₂ III C ₆) uniformly distributed;

Transition zone: no cracks, no pores, no non-metallic inclusions, continuous element gradient;

Hammer handle: ferrite+pearlite structure, grain size ≤ 5 grade.

Judgment basis: in accordance with GB/T 13298 "Method for examination of microstructure of metals".

Composition analysis

Method: Direct reading spectrometer (OES) or chemical titration method;

Required elements: Cr, Mn, Si, C, S, P, Mo, V;

Report requirement: Provide dual spectral reports before and after the furnace, with an error margin of ≤± 0.1%.

Non destructive testing

Method: Ultrasonic testing (UT) or X-ray testing;

Standard: According to GB/T 7233.1 "Ultrasonic Testing of Steel Castings Part 1: General Purpose Steel Castings";

Qualification criteria: No defects such as pores, shrinkage, cracks, etc. with a diameter of ≥ 2mm.

4. International standard reference

ASTM A532/A532M: Standard Specification for Iron Based Wear Resistant Castings

The classification (Class I-IV), chemical composition, hardness, and heat treatment requirements for iron-based wear-resistant castings can be used as a benchmark for material properties, but are not applicable to the design of hammer structures.

ISO 185:2018: Grey iron castings - Specifications

Only applicable to gray cast iron, not suitable for bimetallic composite hammer heads.

Conclusion: Currently, there is no independent standard specifically for "bimetallic hammer heads" internationally. China's GB/T 26652-XXXX is the most systematic and rigorous specification for similar products worldwide.